HullControl Systems FRC Fiberglass Repair Gel Coat Nick or High Spot Repair
1Lightly sand area using 600 grit paperwater

2Wipe down with dry cloth 3Brush on thin film of Aqua Buff 2000 TM 4Buff clean

FRC Fiberglass Repair (HULL) Some hulls are constructed of hand laid fiberglassNormal fiberglass repair and material procedures applyDamaged fiberglass can be easily repaired by following few basic steps1Remove all damaged material with sabre saw or grinder2Using disc grinder or die grinder, taper fiberglass 1" (2.5 cm) back from patch area on inside of part3456"C

Apply masking tape to outside of part to form mold Mix enough polyester resin and catalyst to complete the repair, following instructions for resin being usedApply resin to inside of patch area using disposable paint brush